Ni60Cr23

  • Large image
  • Large image

Chemical Content, %

C P S Mn Si Cr Ni Al Fe Other
Max 0.08 Max 0.02 Max 0.015 Max 0.60 0.75~1.60 20.0~23.0 55-61 Max 0.50 Bal -

Mechanical Properties

Property Name Value
Max Continuous Service Temperature 1150℃
Resistivity ( 20℃) 1.21 mm2 Ω/m
Resistivity ( 20℃) 727 ohm/cmf
Density 8.4 g/cm3
Thermal Conductivity 45.2 KJ/m·h·℃
Coefficient of Thermal Expansion 17×10-6/℃ (20℃~1000℃)
Melting Point 1390℃
Elongation Min 20%
Micrographic Structure Austenite
Magnetic Property nonmagnetic

Temperature Factor of Electrical Resistivity

20℃ 100℃ 200℃ 300℃ 400℃ 500℃ 600℃ 700℃ 800℃ 900℃ 1000℃ 1100℃ 1200℃ 1300℃
1 1.011 1.024 1.038 1.052 1.064 1.069 1.073 1.0278 1.088 1.095 1.109 - -