Resistohm 123
Chemical Content, %
| C | P | S | Mn | Si | Cr | Ni | Al | Fe | Other | 
|---|---|---|---|---|---|---|---|---|---|
| Max 0.08 | Max 0.025 | Max 0.020 | Max 0.50 | ≤0.70 | 18.0~20.0 | ≤0.60 | 2.5-3.5 | Balance | - | 
Mechanical Properties
| Property Name | Value | 
|---|---|
| Max Continuous Service Temp | 1100℃ | 
| Melting Point | 1500℃ | 
| Density | 7.35 g/cm3 | 
| Resisivity at 20℃ | 1.23 μΩ/m | 
| Specific heat | 0.49J(g·K) | 
| Thermal Conductivity | 13 W(m·k) 20℃ | 
| Coefficient of Thermal Expansion | 13.5*10-6 /K(20℃~1000℃) | 
| Tensile Strength | 637~784 Mpa | 
| Elongation | Min 12% | 
| Section Variation Shrink Rate | 65~75% | 
| Repeatedly Bend Frequency | Min 5 times | 
| Fast Life | Min 80h/1250℃ | 
| Hardness | 200-260HB | 
| Micrographic Structure | Ferrite | 
| Magnetic Property | Magnetic | 
Temperature Factor of Electrical Resistivity
| 20℃ | 100℃ | 200℃ | 300℃ | 400℃ | 500℃ | 600℃ | 700℃ | 800℃ | 900℃ | 1000℃ | 1100℃ | 1200℃ | 1300℃ | 
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| 1.000 | 1.011 | 1.025 | 1.042 | 1.061 | 1.085 | 1.120 | 1.142 | 1.154 | 1.164 | 1.172 | 1.180 | 1.186 | - | 